Dura 4024
EN 1.4024

General characteristics

Martensitic grade with slightly increased hardenability (comp. 1.4006). Corrosion resistant in water and steam. For mechanical engineering applications and surgical instruments.

Typical applications

  • Mechanical engineering applications
  • Surgical instruments

 

Product forms, available sizes and finishes

Flat

Product typeFinishesThicknessWidth
Cold rolled coil2B, 2BB, 2C, 2D, 2E, 2G, 2H, 2J, 2R0,05-3,503-1350
Cold rolled sheet2B, 2BB, 2D, 2E, 2G, 2H, 2J0,50-3,50350-1350
Hot rolled coil, pickled1C, 1D, 1G, 1U2,00-8,0030-1530
Precision strip2R0,05-1,503-649
Chemical composition

 

CMnCrNiMoNOther
Typical 0.1613.2
EN 10088-2 0.12-0.17≤1.0012.0-14.0
Mechanical properties

 

 

StandardRp0.2Rp1.0RmElongationImpact strengthRockwellHBHV
 MPaMPaMPa%J
Product type: Cold rolled coil and sheet
EN 10088-2 ≤ 650 ≥ 20
Product type: Hot rolled coil and sheet
EN 10088-2 ≤ 650 ≥ 20

1)Elongation according to EN standard:
A80 for thickness below 3 mm.
A for thickness = 3 mm.
Elongation according to ASTM standard A2” or A50.

Corrosion resistance

 

Pitting corrosion resistanceCrevice corrosion resistance
PRECPTCCT
13

PRE Pitting Resistant Equivalent calculated using the formula: PRE = %Cr + 3.3 x %Mo + 16 x %N
CPT Corrosion Pitting Temperature as measured in the Avesta Cell (ASTM G 150), in a 1M NaCl solution (35,000 ppm or mg/l chloride ions).
CCT Critical Crevice Corrosion Temperature is the critical crevice corrosion temperature which is obtained by laboratory tests according to ASTM G 48 Method F

 

 

Physical properties

 

 

DensityModulus of elasticityThermal exp. at 100 °CThermal conductivityThermal capacityElectrical resistanceMagnetizable
kg/dm3GPa10-6/°CW/m°CJ/kg°CµΩm
7,721610,5304600,60Yes
Fabrication

 

 

Standards & approvals

 

 

StandardDesignation
EN 10088-21.4024